50t电弧炉炼钢TPC技术应用实践

Application and practice of TPC technology in the production of 50t EAF

  • 摘要: 对TPC(Terminal Process Control)技术在50t电弧炉上的应用与实践进行了介绍,对工艺存在的问题进行了分析并介绍了对用氧供电的控制.TPC技术的应用解决了电弧炉高铁水比例冶炼存在的水冷炉盖粘钢、冶炼周期长等工艺问题,使终点成分和温度同时命中率由67%达到91%,各项技术经济指标提升明显,供电时间每炉缩短6min,吨钢冶炼电耗降低58kW·h,电极消耗降低0.3kg,钢材的全氧含量降低.

     

    Abstract: The application condition of TPC (Terminal Process Control) technology in the operation of 50 t EAF were introduced. Through adoption of TPC problems such as steel sticking with water cooled furnace cover were solved, and the hit ratio of predicting both of terminal composition and temperature of the steel increased from 67% to 91%. Additionally, several indicators were greatly improved, for example, the time of electricity supply was shortened by 6 min/furnace, electric consumption was reduced by 58 kW·h·t-1, and electrode con-sumption was reduced by 0.30 kW·h·t-1.

     

/