Ren Huailiang, He Zhaoji, Wang Xuecheng, Zhang Kui. Cobalt-Free Maraging Alloys[J]. Chinese Journal of Engineering, 1987, 9(4): 31-37. DOI: 10.13374/j.issn1001-053x.1987.04.005
Citation: Ren Huailiang, He Zhaoji, Wang Xuecheng, Zhang Kui. Cobalt-Free Maraging Alloys[J]. Chinese Journal of Engineering, 1987, 9(4): 31-37. DOI: 10.13374/j.issn1001-053x.1987.04.005

Cobalt-Free Maraging Alloys

  • The maraging alloys series containing copper but cobalt free have been investigated. It was found that during solid solution treatment, the temperature for the second phase Fe2Mo dissolving completely could not lower than 950℃, and for the alloys containing 6% Mo or less,the recrystallization treatment temperature for high temperature reversed auste-nite was 950℃.For the alloys containing more than 6% Mo, the recrystallization treatment temperature raised with increasing Mo%.Under opi-tical microscopy the morphology after recrystallization was rectangular block shape while it was fine packet shape before recrystallization.
    After solid solution and recrystallization treatments at 950℃ and aging at 540℃ for 3 h, the general mechanical properties of Fe-Nil5-Mo6-Cu4-Ti alloy were as follow:
    σb=1893.3MPa, σ0.2=1784.5MPa.δ5=9.5%, (ψ)=46%,HRC=52.5.
  • loading

Catalog

    /

    DownLoad:  Full-Size Img  PowerPoint
    Return