Preparation and properties of Al2O3/WC-10Co/ZrO2 cermets
-
-
Abstract
Al2O3/WC-10Co/ZrO2 cermets were prepared by a hot-pressing process by using WC 10Co nanocomposite powder, Y2O3 stabilized nanocrystalline ZrO2 powder and submicron Al2O3 powder. The influences of sintering temperature on the microstructure, grain size and properties were investigated according to the density, fracture toughness, Rockwell A hardness (HRA), hysteresis loops and scanning electron microscopy (SEM) micrographs of fractured surfaces of the specimens. The results show that the composite powders (WC-10Co (50%)/Al2O3(40%)/ZrO2(10%)) after being high-energy ball-milled for 48 h was hot-pressing sintered at 1450℃ then submicron Al2O3/WC-10Co/ZrO2 cermets with an average grain size of less than 1μm and better properties of 97.5% in relative density, 7. 446 8 Ma·m1/2 in fracture toughness, HRA 94.0 is achieved.
-
-